GLAÇURES à CÔNE 6 en RÉDUCTION

par Diana PANCIOLI

RECETTE N°13

 
 

  

FICHE N° 13

Nom de la Recette : BLEU MAT PÂLE

Cône : 6

Aspect : MAT

Couleur : TURQUOISE PÂLE

Cuisson : REDUCTION

Ingrédients :

%

Feldspath Custer

55.0

Kaolin EPK

14.0

Silice

7.0

Craie

24.0

Total :

100.0

Ajouts :

%

Carbonate de cobalt

0.5

Carbonate de cuivre

3.0

Rutile

6.0

Bentonite

2.0

Seger
% poids
% Molaire

Li2O

-
-
-

Na2O

0.081
1.92
2.03

K2O

0.180
6.44
4.48

MgO

0.006
0.09
0.14

CaO

0.733
15.66
18.30

SrO

-
-
-

BaO

-
-
-

ZnO

-
-
-

PbO

-
-
-

S/total Alcalins

0.261
8.36
6.51

total des fondants

1.000
24.11
24.95

Al2O3

0.435
16.87
10.84

B2O3

-
-
-

Fe2O3

0.004
0.23
0.10

SiO2

2.567
58.72
64.06

TiO2

0.002
0.05
0.04

P2O5

0.000
0.02
0.01

SiO2/Al2O3

5.91

Coef. Dilat.

83.49

Perte au feu

13.07

Coût en $ par livre de glaçure :

0.83

Photo de la glaçure

Commentaires :

Dérivé du «Bronze/Vert Mat» de Rick Malgrem.
Un bleu pâle qui devient gris plus foncé dans les endroits profonds.
Trop mate pour être employée comme revêtement intérieur.
Une application moyenne est suggérée.
 
 
 

MATIÈRES NORD-AMÉRICAINES UTILISÉES DANS CES RECETTES :

 
FRITTES :
Ferro 3110 : K2O 0,064 Na2O 0,644 CaO 0,293 Al2O3 0,095 B2O3 0,097 SiO2 3,003
Fritte Ferro 3134 : Na2O 0,317 CaO 0,683 B2O3 0,634 SiO2 1,476
Fritte Ferro 3195 : Na2O 0,313 CaO 0,686 Al2O3 0,404 B2O3 1,099 SiO2 2,751
 
 
Matières premières et équivalents Européens :
 
Kentuky OM#4 ball clay (Old Mine #4): OM #4 is a fine-grained ball clay with good plasticity and strength. It is very common in glaze recipes. It undergoes a sudden color shift around cone 8-9, from straw yellow to solid gray [IMC]. Composition % 0.3 Na2O 1.0 K2O 0.4 MgO 0.3 CaO 27.9 Al2O3 55.2 SiO2 1.2 TiO2 1.1 Fe2O3 12.6 Perte au feu.
 
Kona F4 Feldspar : Commonly used soda feldspar; used in porcelains because of its low iron content. Composition % 6.90 Na2O 4.8 K2O 0.05 MgO 1.70 CaO 19.60 Al2O3 66.80 SiO2 0.04 Fe2O3 0.20 Perte au feu = Feldspath CR-79 (DAM - IMERYS)
 
Custer Feldspar : Commonly used potash feldspar. Can be used to substitute for Keystone, BuckinghamFeldspath CR-79 (DAM) , Yankee, or Kingman feldspars. Composition % 2.91 Na2O 10.28 K2O 0.30 CaO 17.35 Al2O3 69.00 SiO2 0.12 Fe2O3 0.04 Perte au feu = Feldspath ICE 10B (DAM - IMERYS)
 
Epsom salts : magnesium sulfate. Highly soluble; used in small quantities (0.1%-1%) as a flocculant in slips and glazes. Many sources recommend making a concentrated solution, then adding the solution to the mixed glaze. Composition Molaire : MgO SO3 7 H2O.
 
Argile Red Art : An iron-rich clay consisting of clay/shale deposits from a prehistoric lake bed. Contains 40% illite, 10% kaolinite, 7% iron oxide, and 15% mixed layered clays. Composition % 0.38 Na2O 4.15 K2O 1.59 MgO 0.26 CaO 15.51 Al2O3 64.95 SiO2 1.09 TiO2 7.05 Fe2O3 0.22 P2O5 4.80 Perte au feu.
 
Cornwall stone : Composition % 3.30 Na2O 4.31 K2O 0.14 MgO 1.81 CaO 16.31 Al2O3 73.80 SiO2 0.15 TiO2 0.20 Fe2O3
 
Spodumène Foote : Composition % Li2O 7.26 SiO2 63.84 Al2O3 28.61 Fe2O3 0.19 CaO 0.04 MgO trace Perte au feu 0.16
 
EPK Kaolin (Edgar Plastic Kaolin, origine Floride) : CaO 0.18 MgO 0.10 K2O 0.33 Na2O 0.06 P2O5 0.24 TiO2 0.37 Al2O3 37.36 SiO2 45.73 Fe2O3 0.79 Perte au feu 13.20
 
 
 
Smart2000.fr © Avril 2009 - FRANCE
Contact : Smart2000@wanadoo.fr
Document pour CONSULTATION PRIVÉE uniquement - Toute reproduction totale ou partielle est interdite
 
 

 
Smart2000.fr le site dédié aux passionnés de céramique
 
Smart2000 - FRANCE sur https://smart2000.fr/
 
This entire page Copyright © 2009-2023, All Rights Reserved.
Les textes et les photos restent la propriété de leur auteurs, ils ne peuvent être réutilisés sans un accord préalable. Nous consulter.
 
Sommaire